molybdenum & chrome molybdenum heat-resistant steel electrode |
electrode brand
|
GB
|
AWS
|
coated type
|
power supply
|
main application
|
specification
|
AH-R107
|
E5015-A1
|
E7015-A1
|
low-hydrogen type
|
DC
|
used for welding pearlitic heat-resisting steel such as 15Mo with working temperature below 510℃ |
Ø3.2-Ø5.0
|
AH-R207
|
E5515-B1
|
E8015-B1
|
low-hydrogen type
|
DC
|
used for welding pearlitic heat-resisting steel such as 12CrMo with working temperature below 510℃ |
Ø3.2-Ø5.0
|
AH-R307
|
E5515-B2
|
E8015-B2
|
low hydrogen sodium type
|
DC
|
used for welding pearlitic heat-resisting steel such as 15CrMo with working temperature below 520℃ |
Ø3.2-Ø5.0
|
AH-R317
|
E5515-B2-V
|
|
low hydrogen sodium type
|
DC
|
used for welding pearlitic heat-resisting steel such as 12CrMoV with working temperature below 540℃ |
Ø3.2-Ø5.0
|
AH-R327
|
E5515-B2-VW
|
|
low hydrogen sodium type
|
DC
|
used for welding pearlitic heat-resisting steel such as 15CrMoV with working temperature below 570℃ |
Ø3.2-Ø5.0
|
AH-R337
|
E5515-B2-VNb
|
|
low hydrogen sodium type
|
DC
|
Ø3.2-Ø5.0
|
AH-R347
|
E5515-B2-VWB
|
|
low hydrogen sodium type
|
DC
|
used for welding pearlitic heat-resisting steel with working temperature below 620℃ |
Ø3.2-Ø5.0
|
AH-R407
|
E6015-B3
|
E9015-B3
|
low hydrogen sodium type
|
DC
|
used for welding Cr2·5Mo pearlitic heat-resisting steel |
Ø3.2-Ø5.0
|
AH-R417
|
E5515-B3-VNb
|
|
low hydrogen sodium type
|
DC
|
used for welding pearlitic heat-resisting steel such as 12Cr3MoVSiTiB |
Ø3.2-Ø5.0
|
AH-R507
|
E5MoV-15
|
|
low hydrogen sodium type
|
DC
|
used for welding pearlitic heat-resisting steel such as Cr5Mo |
Ø3.2-Ø5.0
|
AH-R707
|
E9Mo-15
|
|
low hydrogen sodium type
|
DC
|
used for welding Cr9Mo heat-resisting steel and superheater pipeline |
|
AH-R802
|
E11MoVNi-16
|
|
lime-titania type |
AC,DC
|
used for welding 1Cr11MoV heat-resisting steel with working temperature below 565℃ |
Ø3.2-Ø5.0
|
AH-R807
|
E11MoVNi-15
|
|
low hydrogen sodium type
|
DC
|
Ø3.2-Ø5.0
|
electrode brand
|
chemical composition of deposited metal % |
mechanical performance of deposited metal |
C
|
Mn
|
Si
|
Cr
|
Mo
|
V
|
W
|
B
|
S
|
P
|
Nb
|
Ni
|
tensile strength Mpa |
yield strength Mpa |
elongation % |
impact value ℃ |
impact value J |
AH-R107
|
0,086
|
0,68
|
0,42
|
|
0,52
|
|
|
|
0,014
|
0,019
|
|
|
563
|
452
|
28
|
normal temperature
|
126
|
AH-R207
|
0,080
|
0,72
|
0,44
|
0,51
|
0,57
|
|
|
|
0,015
|
0,018
|
|
|
573
|
456
|
25,7
|
normal temperature
|
130
|
AH-R307
|
0,076
|
0,81
|
0,50
|
1,12
|
0,55
|
|
|
|
0,014
|
0,020
|
|
|
573
|
470
|
25,6
|
normal temperature
|
128
|
AH-R317
|
0,072
|
0,78
|
0,41
|
1,30
|
0,54
|
0,21
|
|
|
0,020
|
0,021
|
|
|
586
|
460
|
28,6
|
normal temperature
|
142
|
AH-R327
|
0,081
|
0,88
|
0,43
|
1,25
|
0,82
|
0,28
|
0,32
|
|
0,018
|
0,020
|
|
|
638
|
508
|
23,5
|
normal temperature
|
158
|
AH-R337
|
0,064
|
0,78
|
0,40
|
1,31
|
0,88
|
0,31
|
|
|
0,017
|
0,022
|
0,18
|
|
593
|
461
|
24,0
|
normal temperature
|
144
|
AH-R347
|
0,076
|
0,84
|
0,45
|
2,10
|
0,50
|
0,36
|
0,41
|
0,002
|
0,014
|
0,019
|
|
|
578
|
455
|
26,0
|
normal temperature
|
131
|
AH-R407
|
0,082
|
0,78
|
0,44
|
2,24
|
1,02
|
|
|
|
0,015
|
0,019
|
|
|
620
|
544
|
25,3
|
normal temperature
|
156
|
AH-R417
|
0,083
|
0,80
|
0,41
|
2,68
|
0,87
|
0,35
|
|
|
0,016
|
0,020
|
0,41
|
|
586
|
462
|
24
|
normal temperature
|
145
|
AH-R507
|
0,081
|
0,76
|
0,32
|
5,80
|
0,57
|
0,24
|
|
|
0,018
|
0,021
|
|
|
590
|
|
21,8
|
|
|
AH-R707
|
0,10
|
0,83
|
0,30
|
9,40
|
0,83
|
|
|
|
0,014
|
0,015
|
|
|
625
|
|
20,4
|
|
|
AH-R802
|
0,13
|
0,87
|
0,33
|
10,2
|
0,67
|
0,30
|
|
|
0,015
|
0,016
|
|
0,78
|
785
|
|
18,8
|
|
|
AH-R807
|
0,12
|
0,88
|
0,34
|
10,4
|
0,80
|
0,33
|
|
|
0,013
|
0,015
|
|
0,80
|
808
|
|
19,0
|
|
|